ASTM A334 / ASME SA334 Grade 6 Specification Summary
This page summarises the requirements of ASTM A334 / ASME SA334, Seamless and Welded Carbon and Alloy-Steel Tubes for Low-Temperature Service, for Grade 6, the killed carbon steel grade impact tested at −45 °C (−50 °F). Always check the edition named in your purchase order.
To buy low-temperature tubes, see our ASTM A334 tubes page and, for pipe, low-temperature carbon steel pipes to ASTM A333.
A printable version is available as the ASTM A334 Grade 6 tube specification sheet (PDF).
Scope of ASTM A334
| Item | Requirement |
|---|---|
| Title | Seamless and welded carbon and alloy-steel tubes for low-temperature service |
| Product | Minimum-wall-thickness tubes for use at low temperatures |
| Grades | 1, 3, 6, 7, 8, 9 and 11 (Grade 6: killed carbon steel) |
| Types | Seamless or welded |
| Mechanical properties | Do not apply to tubing under 3.2 mm (1/8 in) OD or 0.4 mm (0.015 in) wall |
| General requirements | ASTM A1016 / ASME SA1016 |
Manufacture and Heat Treatment
- Process: seamless or welded, as ordered.
- Grade 6 heat treatment: normalised; or normalised and tempered; or, for seamless tubes, hot finishing in a controlled temperature range and cooling from the finishing temperature, as the specification allows.
- Purpose: heat treatment controls the microstructure so the tubes meet the −45 °C impact test.
A334 Grade 6 Chemical Composition (%)
| Element | Grade 6 |
|---|---|
| Carbon, max | 0.30 |
| Manganese | 0.29–1.06 |
| Phosphorus, max | 0.025 |
| Sulphur, max | 0.025 |
| Silicon, min | 0.10 |
For each reduction of 0.01% carbon below 0.30%, an increase of 0.05% manganese above 1.06% is permitted, up to 1.35% manganese.
A334 Grade 6 Mechanical Properties
| Property | Requirement |
|---|---|
| Tensile strength, min | 415 MPa (60 ksi) |
| Yield strength, min | 240 MPa (35 ksi) |
| Elongation in 50 mm, min | 30% longitudinal; 16.5% transverse |
Impact Test Requirements
| Specimen | Min. average of 3 | Min. single value |
|---|---|---|
| Full size 10 × 10 mm | 18 J (13 ft-lbf) | 14 J (10 ft-lbf) |
| Sub-size | Reduced values per the specification table | Reduced values per the specification table |
Charpy V-notch test temperature for Grade 6: −45 °C (−50 °F). Tubes too small for sub-size specimens are covered by the specification’s alternative rules.
Dimensional Tolerances (ASTM A1016)
| Outside diameter | OD tolerance (cold finished) |
|---|---|
| Under 25.4 mm (1 in) | ±0.10 mm |
| 25.4 to 38.1 mm (1 to 1½ in), incl. | ±0.15 mm |
| Over 38.1 to under 50.8 mm | ±0.20 mm |
| 50.8 to under 63.5 mm | ±0.25 mm |
| 63.5 to under 76.2 mm | ±0.30 mm |
| 76.2 to 101.6 mm, incl. | ±0.38 mm |
| Over 101.6 mm | +0.38 / −0.64 mm |
Wall thickness: A334 is a minimum-wall specification, so the wall may be over the ordered minimum but not under it. Under A1016 the plus tolerance is about +18% for welded tubes and +20% to +22% for cold-finished seamless tubes; hot-finished seamless tubes have larger allowances.
Required Tests
- Tension test per lot
- Flattening test per lot
- Flaring test (seamless) or flange and reverse flattening tests (welded)
- Charpy V-notch impact test at −45 °C
- Hydrostatic or nondestructive electric test on every tube
Related Grades
| Specification | Product | Main difference from A334 Gr 6 |
|---|---|---|
| A334 Grade 1 | Low-temperature CS tubes | Lower strength (380/205 MPa); no silicon minimum |
| A333 Grade 6 | Low-temperature CS pipe | Same chemistry and impact test; pipe sizes (NPS, schedule) |
| SA179 (spec) | Seamless CS heat-exchanger tubes | No impact test; not for low-temperature service |
| SA192 (spec) | Seamless CS boiler tubes | High-pressure boiler service; no impact test |
Ordering Information
An A334 order should state: quantity; grade (6); seamless or welded; size (OD and minimum wall); length; impact test temperature if lower than standard; optional requirements such as product analysis; certificates (EN 10204 3.1 or as required); and the specification number and edition.
Need A334 Grade 6 tubes? Send the OD, minimum wall, seamless or welded, length and quantity to kamlesh@dineshtube-india.com or call +91 83559 10913. You can also send an enquiry.
This is a summary for reference only. ASTM A334/A334M and ASME SA-334 are copyrighted standards; the purchased standard and the edition on the order govern.
ASTM A334 Grade 6 Tube Specification (ASME SA334): FAQs
What does ASTM A334 cover?
ASTM A334 / ASME SA334 covers several grades of minimum-wall-thickness, seamless and welded, carbon and alloy-steel tubes intended for use at low temperatures. Grade 6 is the most widely used carbon steel grade, impact tested at −45 °C (−50 °F).
What is the chemical composition of A334 Grade 6?
Carbon 0.30% max, manganese 0.29–1.06%, phosphorus 0.025% max, sulphur 0.025% max and silicon 0.10% min. For each 0.01% reduction in carbon below 0.30%, manganese may be raised by 0.05% above 1.06%, up to 1.35%.
What are the mechanical properties of A334 Grade 6?
Minimum tensile strength 415 MPa (60 ksi), minimum yield strength 240 MPa (35 ksi), and minimum elongation 30% longitudinal or 16.5% transverse in 50 mm.
What impact test does A334 Grade 6 need?
Charpy V-notch tests at −45 °C (−50 °F). For full-size specimens the average of three must be at least 18 J (13 ft-lbf) and no single value below 14 J (10 ft-lbf); lower values apply to sub-size specimens.
What is the difference between A334 Grade 6 and A333 Grade 6?
The chemistry, tensile and impact requirements are essentially the same. A334 covers tubes ordered by OD and minimum wall, for heat exchangers and similar uses; A333 covers pipe ordered by NPS and schedule.
A334 Grade 1 or Grade 6?
Both are impact tested at −45 °C. Grade 6 has higher strength (415/240 MPa against 380/205 MPa) and a silicon minimum (killed steel), so it is the usual choice for low-temperature heat exchanger tubes; Grade 1 is a lower-strength alternative.